Click here to make tpub.com your Home Page

Page Title: Table III. rolled carbon spring steel, cast or heat chemical Ranges and Limits
Back | Up | Next

Click here for thousands of PDF manuals

Google


Web
www.tpub.com

Home

   
Information Categories
.... Administration
Advancement
Aerographer
Automotive
Aviation
Construction
Diving
Draftsman
Engineering
Electronics
Food and Cooking
Logistics
Math
Medical
Music
Nuclear Fundamentals
Photography
Religion
   
   

 




img
III.
rolled carbon spring steel, cast or heat chemical
ranges and limits.
Standard chemical ranges and limits, percent
Lowest
When
of specified
Element
Range
element
Carbon
Over 0.60 t o 0.80
0.11
0.60
Note
Over
to 1.35
Manganese
To 0.50
0.20
0.40
Over 0.50 to 1.15
over 1.15 to 1.65
Phosphorus
To 0.08
0.03
0.04
Over 0.08 to 0.15
To 0.08
0.05
Over 0.08 to C.15 fncl.
l 05
Over
to
l 07
Over
to
l
Silicon
0.10
To 0.15
0.08
Over 0.15 to 0.30
Over
to . 60
Copper
When copper is required
0.20 minimum is
specified
The carbon ranges shown in the column headed "Range" apply
Note 1. Carbon:
when the specified maximum limit for manganese does not
exceed 1.00 percent.  When the maximum manganese
exceeds 1.00 percent, add 0.01 to the carbon rangaes shown
above.